Crack Width to EC2: Calculating wk Step by Step

Eurocode 2 limits crack width to 0.3 mm for most reinforced concrete, but the calculation behind that number is rarely shown in full. This article works through §7.3.4 from the cracked section analysis to the final wk: how the maximum crack spacing is built from cover and bar diameter, why the effective tension area is not the whole section, what the 0.6 floor on the strain difference is protecting, and a complete 300 by 600 beam check with every intermediate value.

20 October 2026
Reviewed by CivilAxis editors
Cracked concrete around a corroding steel bar, with rust staining at the crack
Photo: JonRichfield / Wikimedia Commons, CC BY-SA 3.0

A crack in reinforced concrete is not a defect. Reinforced concrete works by cracking: the concrete lets go of the tension, the steel picks it up, and the member carries on. What the code controls is not whether the section cracks but how wide the cracks open, because width is what governs durability, water-tightness and whether the owner thinks the structure is broken.

What the check does

EN 1992-1-1 §7.3.1 asks that the calculated crack width stays under a limit that depends on the exposure class and on whether the member is prestressed:

wk≤wmaxw_k \le w_{max}

Table 7.1N recommends wmax=0.3 mmw_{max} = 0.3\ \mathrm{mm} for reinforced members in exposure classes XC2 to XS3, checked under the quasi-permanent combination. For X0 and XC1 the recommendation relaxes to 0.4 mm, since the concern there is appearance rather than durability. Prestressed members with bonded tendons are tighter: 0.2 mm, and under the frequent combination.

Three things are worth saying before any arithmetic. The limit is a durability and appearance limit, not a strength limit - a member with a 0.35 mm crack is no weaker. The calculated wkw_k is a characteristic value with real scatter around it, so treating 0.31 against 0.30 as a hard pass or fail is reading more precision into the model than it has. And §7.3.3 offers a simplified route: satisfy the bar diameter or bar spacing limits of Table 7.3N and no calculation is needed at all.

The governing formula

wk=sr,max (εsm−εcm)w_k = s_{r,max}\,(\varepsilon_{sm} - \varepsilon_{cm})

where:

  • wkw_k - characteristic crack width (mm)

  • sr,maxs_{r,max} - maximum crack spacing (mm)

  • εsm\varepsilon_{sm} - mean strain in the reinforcement under the relevant combination, including the effect of imposed deformations and tension stiffening

  • εcm\varepsilon_{cm} - mean strain in the concrete between cracks

The shape of it is simply geometry: a crack opens by the amount the steel stretches more than the concrete does, over the length of concrete that belongs to that crack. Everything else in §7.3.4 is working out those two quantities.

Step 1 - the cracked section

Before anything in §7.3.4 can be evaluated, you need the steel stress under the quasi-permanent combination. That comes from a cracked transformed section analysis: assume the concrete carries no tension, find the neutral axis depth xx where the compressive and tensile first moments balance, then take the second moment of area of what is left.

b x22+αeAs2(x−d2)=αeAs1(d−x)\frac{b\,x^2}{2} + \alpha_e A_{s2}(x - d_2) = \alpha_e A_{s1}(d - x)

Icr=b x33+αeAs1(d−x)2+αeAs2(x−d2)2I_{cr} = \frac{b\,x^3}{3} + \alpha_e A_{s1}(d - x)^2 + \alpha_e A_{s2}(x - d_2)^2

where:

  • xx - neutral axis depth measured from the compression face (mm)

  • αe=Es/Ecm\alpha_e = E_s / E_{cm} - modular ratio

  • As1A_{s1}, As2A_{s2} - tension and compression steel areas (mm2\mathrm{mm^2})

  • dd, d2d_2 - effective depths to the tension and compression steel (mm)

  • IcrI_{cr} - second moment of area of the cracked transformed section (mm4\mathrm{mm^4})

The steel stress then follows from ordinary elastic bending:

σs=αeMqp (d−x)Icr\sigma_s = \alpha_e \frac{M_{qp}\,(d - x)}{I_{cr}}

One decision hides in αe\alpha_e. For a short-term check, EcmE_{cm} is the tabulated secant modulus. For the quasi-permanent combination, which is a long-term state, an effective modulus Ec,eff=Ecm/(1+φ)E_{c,eff} = E_{cm} / (1 + \varphi) is more honest, and the creep coefficient φ\varphi can easily be 2. That raises αe\alpha_e from about 6 to about 18, pushes the neutral axis down, and increases the crack width. The example below uses the short-term modulus so that each step can be followed; a real design should decide this question explicitly rather than inherit it from a default.

Step 2 - maximum crack spacing

sr,max=k3c+k1k2k4ϕρp,effs_{r,max} = k_3 c + \frac{k_1 k_2 k_4 \phi}{\rho_{p,eff}}

where:

  • cc - clear cover to the longitudinal reinforcement (mm)

  • ϕ\phi - bar diameter, or an equivalent diameter for a mixed bundle (mm)

  • k1k_1 - bond coefficient: 0.8 for high bond bars, 1.6 for bars with an effectively plain surface

  • k2k_2 - strain distribution coefficient: 0.5 for bending, 1.0 for pure tension

  • k3k_3 - recommended value 3.4

  • k4k_4 - recommended value 0.425

  • ρp,eff=As/Ac,eff\rho_{p,eff} = A_s / A_{c,eff} - the reinforcement ratio in the effective tension area

The two terms say different things. k3ck_3 c is the distance the bond has to travel before it can start transferring force at all, so deeper cover means wider cracks - which is the uncomfortable trade-off at the heart of durability design. The second term is the bond transfer length: more steel in the tension zone, or smaller bars at the same area, means shorter transfer and closer, finer cracks.

Ac,effA_{c,eff} is the concrete around the bars that actually participates, not the whole tension zone. Its depth is

hc,ef=min⁡(2.5 (h−d), h−x3, h2)h_{c,ef} = \min\left(2.5\,(h - d),\ \frac{h - x}{3},\ \frac{h}{2}\right)

For a beam of ordinary proportions the first term usually wins, which makes hc,efh_{c,ef} a small band around the bars. That is deliberate: the tension stiffening effect is local to the bars.

Where the bar spacing exceeds 5(c+ϕ/2)5(c + \phi/2), the bars are too far apart for that model and the code falls back to an upper bound sr,max=1.3 (h−x)s_{r,max} = 1.3\,(h - x).

Step 3 - the strain difference

εsm−εcm=σs−ktfct,effρp,eff(1+αeρp,eff)Es ≥ 0.6 σsEs\varepsilon_{sm} - \varepsilon_{cm} = \frac{\sigma_s - k_t \dfrac{f_{ct,eff}}{\rho_{p,eff}}\left(1 + \alpha_e \rho_{p,eff}\right)}{E_s} \ \ge\ 0.6\,\frac{\sigma_s}{E_s}

where:

  • σs\sigma_s - steel stress at the crack, from the cracked section (MPa)

  • ktk_t - 0.6 for short-term loading, 0.4 for long-term

  • fct,efff_{ct,eff} - concrete tensile strength at the time cracking is expected, normally fctmf_{ctm} (MPa)

  • EsE_s - 200 000 MPa

The subtracted term is tension stiffening: between cracks the concrete is still gripping the bar, so the steel's average strain is lower than its strain at the crack face. kt=0.4k_t = 0.4 for long-term loading because sustained load and creep gradually break that grip down.

The 0.6 σs/Es0.6\,\sigma_s / E_s floor is the part that is easy to miss. At low steel stress the tension stiffening term can swallow the whole numerator and hand back a negative, physically meaningless strain difference. The floor stops that, and it means a lightly stressed member never reports a crack width of zero.

Minimum reinforcement is the other half of §7.3

§7.3.2 is not optional and it is not the same check:

As,min σs=kc k fct,eff ActA_{s,min}\,\sigma_s = k_c\,k\,f_{ct,eff}\,A_{ct}

where:

  • ActA_{ct} - area of concrete in the tension zone just before the first crack (mm2\mathrm{mm^2})

  • kck_c - stress distribution coefficient: 0.4 for bending, 1.0 for pure tension

  • kk - allowance for self-equilibrating stresses: 1.0 for webs up to 300 mm, 0.65 for webs 800 mm or more, interpolated between

  • σs\sigma_s - steel stress allowed at the crack, often taken as fykf_{yk}

The logic is that the steel must be able to carry the force the concrete released at the moment it cracked. If it cannot, the first crack does not stabilise into a pattern of fine cracks - it keeps opening. A section can pass the wkw_k calculation and still fail this, because the two checks ask different questions.

Worked example

Section: 300 mm wide, 600 mm deep, C30/37, B500. Tension steel 3 bars of 20 mm, centres 40 mm from the soffit. Compression steel 2 bars of 12 mm, centres 40 mm from the top. Clear cover to the main bars c=30 mmc = 30\ \mathrm{mm}. Quasi-permanent moment Mqp=150 kN⋅mM_{qp} = 150\ \mathrm{kN \cdot m}, no axial force. Limit wmax=0.3 mmw_{max} = 0.3\ \mathrm{mm}.

Materials.

fctm=0.30 fck2/3=0.30×302/3=2.90 MPaf_{ctm} = 0.30\,f_{ck}^{2/3} = 0.30 \times 30^{2/3} = 2.90\ \mathrm{MPa}

Ecm=22000(fcm10)0.3=22000×3.80.3=32 837 MPaE_{cm} = 22000\left(\frac{f_{cm}}{10}\right)^{0.3} = 22000 \times 3.8^{0.3} = 32\,837\ \mathrm{MPa}

αe=200 00032 837=6.09\alpha_e = \frac{200\,000}{32\,837} = 6.09

Cracked section. With d=560 mmd = 560\ \mathrm{mm} and As1=942 mm2A_{s1} = 942\ \mathrm{mm^2}:

x=125.8 mmIcr=1.29×109 mm4x = 125.8\ \mathrm{mm} \qquad I_{cr} = 1.29 \times 10^{9}\ \mathrm{mm^4}

σc=Mqp xIcr=150×106×125.81.29×109=14.6 MPa\sigma_c = \frac{M_{qp}\,x}{I_{cr}} = \frac{150 \times 10^{6} \times 125.8}{1.29 \times 10^{9}} = 14.6\ \mathrm{MPa}

σs=αeMqp(d−x)Icr=6.09×150×106×434.21.29×109=307 MPa\sigma_s = \alpha_e \frac{M_{qp}(d - x)}{I_{cr}} = 6.09 \times \frac{150 \times 10^{6} \times 434.2}{1.29 \times 10^{9}} = 307\ \mathrm{MPa}

The concrete stress is worth a glance on its own: §7.2 recommends keeping σc\sigma_c below 0.45 fck=13.5 MPa0.45\,f_{ck} = 13.5\ \mathrm{MPa} under the quasi-permanent combination if linear creep is to be assumed, and 14.6 MPa is just over it. In a real design that is a prompt to use non-linear creep or to revisit the section, not a failure.

Effective tension area.

hc,ef=min⁡(2.5×40, 600−125.83, 300)=min⁡(100, 158, 300)=100 mmh_{c,ef} = \min\left(2.5 \times 40,\ \frac{600 - 125.8}{3},\ 300\right) = \min(100,\ 158,\ 300) = 100\ \mathrm{mm}

Ac,eff=300×100=30 000 mm2A_{c,eff} = 300 \times 100 = 30\,000\ \mathrm{mm^2}

ρp,eff=94230 000=0.0314\rho_{p,eff} = \frac{942}{30\,000} = 0.0314

Crack spacing. High bond bars in bending, so k1=0.8k_1 = 0.8 and k2=0.5k_2 = 0.5:

sr,max=3.4×30+0.8×0.5×0.425×200.0314=102+108=210 mms_{r,max} = 3.4 \times 30 + \frac{0.8 \times 0.5 \times 0.425 \times 20}{0.0314} = 102 + 108 = 210\ \mathrm{mm}

Strain difference. Long-term, so kt=0.4k_t = 0.4:

εsm−εcm=307−0.4×2.900.0314 (1+6.09×0.0314)200 000=307−43.9200 000=1.32×10−3\varepsilon_{sm} - \varepsilon_{cm} = \frac{307 - 0.4 \times \dfrac{2.90}{0.0314}\,(1 + 6.09 \times 0.0314)}{200\,000} = \frac{307 - 43.9}{200\,000} = 1.32 \times 10^{-3}

The floor is 0.6×307/200 000=0.92×10−30.6 \times 307 / 200\,000 = 0.92 \times 10^{-3}, which is lower, so the calculated value governs.

Crack width.

wk=210×1.32×10−3=0.28 mmw_k = 210 \times 1.32 \times 10^{-3} = 0.28\ \mathrm{mm}

Result: wk=0.28 mm≤0.3 mmw_k = 0.28\ \mathrm{mm} \le 0.3\ \mathrm{mm}, so the section passes, with about 8% in hand. The margin is thin enough that the creep assumption matters: repeat the check with an effective modulus and the steel stress rises, and so does wkw_k.

It is also worth noticing what the simplified route would have said. At σs=307 MPa\sigma_s = 307\ \mathrm{MPa} and wmax=0.3 mmw_{max} = 0.3\ \mathrm{mm}, Table 7.3N allows a maximum bar diameter of roughly 9 mm or a maximum spacing of roughly 166 mm. The provided bars are 20 mm at about 100 mm spacing, so the spacing limit is satisfied and the diameter limit is not. Either one is sufficient under §7.3.3, and in any case the direct calculation of §7.3.4 supersedes both.

Key points

  • wk=sr,max(εsm−εcm)w_k = s_{r,max}(\varepsilon_{sm} - \varepsilon_{cm}): crack opening is the extra steel stretch over the length of concrete belonging to one crack.

  • Deeper cover gives wider cracks through the k3ck_3 c term. Durability and crack control pull in opposite directions and the code lets both apply.

  • Smaller bars at the same steel area give finer cracks, because ϕ/ρp,eff\phi / \rho_{p,eff} falls.

  • Ac,effA_{c,eff} is a shallow band around the bars, not the whole tension zone.

  • The 0.6 σs/Es0.6\,\sigma_s / E_s floor stops tension stiffening from returning a negative strain difference at low stress.

  • Decide the modular ratio deliberately. Using the short-term EcmE_{cm} under a quasi-permanent combination is optimistic.

  • §7.3.2 minimum reinforcement is a separate check with its own failure mode, and passing wkw_k does not cover it.

References

  1. EN 1992-1-1:2004 - Design of concrete structures - Part 1-1 - §7.3.1 Crack control, general considerations
  2. EN 1992-1-1:2004 - §7.3.2 Minimum reinforcement areas
  3. EN 1992-1-1:2004 - §7.3.3 Control of cracking without direct calculation, Table 7.3N
  4. EN 1992-1-1:2004 - §7.3.4 Calculation of crack widths